Steel Plate GB/T1591
GB/T1591 Q345A
C % |
Si % |
Mn % |
P % |
S % |
N % |
≤0.16 |
≤0.55 |
0.80-1.50 |
≤0.040 |
≤0.040 |
… |
Thickness |
Yield Strength (Mpa) |
Tensile Strength |
Elongation |
Impact Energy |
(mm) |
(MPa) |
(%) |
Min |
≤ 16 |
295 |
390-570 |
23 |
+20℃ |
34J |
> 16-40 |
275 |
390-570 |
23 |
+20℃ |
34J |
>40 |
255 |
390-570 |
23 |
+20℃ |
34J |
The min impact energy is longitudinal energy |
GB/T1591 Q390A
C % |
Si % |
Mn % |
P % |
S % |
N % |
≤0.20 |
≤0.55 |
1.00-1.60 |
≤0.045 |
≤0.045 |
… |
Thickness |
Yield Strength (Mpa) |
Tensile Strength |
Elongation |
Impact Energy |
(mm) |
(MPa) |
(%) |
Min |
≤ 16 |
390 |
490-650 |
19 |
- |
- |
> 16-35 |
370 |
490-650 |
19 |
- |
- |
>35 |
350 |
490-650 |
19 |
- |
- |
The min impact energy is longitudinal energy |
GB/T1591 Q420B
C % |
Si % |
Mn % |
P % |
S % |
N % |
≤0.20 |
≤0.55 |
1.00-1.70 |
≤0.040 |
≤0.040 |
… |
Thickness |
Yield Strength (Mpa) |
Tensile Strength |
Elongation |
Impact Energy |
(mm) |
(MPa) |
(%) |
Min |
≤ 16 |
420 |
520-680 |
18 |
20 |
34 |
> 16-35 |
400 |
520-680 |
18 |
20 |
34 |
>35 |
380 |
520-680 |
18 |
20 |
34 |
The min impact energy is longitudinal energy |
GB/T1591 Q460E
C % |
Si % |
Mn % |
P % |
S % |
N % |
≤0.20 |
≤0.55 |
1.00-1.70 |
≤0.025 |
≤0.025 |
… |
Thickness |
Yield Strength (Mpa) |
Tensile Strength |
Elongation |
Impact Energy |
(mm) |
(MPa) |
(%) |
Min |
≤ 16 |
460 |
550-720 |
17 |
-40 |
27 |
> 16-35 |
440 |
550-720 |
17 |
-40 |
27 |
>35 |
420 |
550-720 |
17 |
-40 |
27 |
The min impact energy is longitudinal energy |
If you are interested in other carbon steel plates, please click here - ASTM A36, ASTM A283, ASTM A572, ASTM A656, JIS G3101 SS400, EN10025-2, DIN 17100, DIN 17102, GB/T700.